The table our own engineers keep on the wall. Names differ between Chinese and Western standards; the metals behind them, as we stock them, are cross-referenced here with the heat chemistry on the MTR.
| Common name | ASTM / UNS | GB (China) | EN / W.Nr. | JIS | Typical use |
|---|---|---|---|---|---|
| Ni200 | N02200 | N6 | 2.4060 | NW2200 | Commercially pure nickel, general |
| Ni201 | N02201 | N4 | 2.4061 | NW2201 | Low-carbon nickel, above 315 °C |
| Inconel 600 | N06600 | GH600 | 2.4816 | NCF600 | Furnace fixtures, caustic |
| Inconel 601 | N06601 | GH601 | 2.4851 | NCF601 | Oxidation to 1,200 °C |
| Inconel 625 | N06625 | GH625 | 2.4856 | NCF625 | Marine, chemical, bellows |
| Inconel 718 | N07718 | GH4169 | 2.4668 | NCF718 | Fasteners, springs, age hardened |
| Inconel X-750 | N07750 | GH145 | 2.4669 | NCF750 | Springs and seals to 700 °C (continuous) |
| Monel 400 | N04400 | — | 2.4360 | NW4400 | Ni-Cu, seawater, HF acid |
| Monel K500 | N05500 | — | 2.4375 | — | Age-hardened Ni-Cu |
| Hastelloy C-276 | N10276 | — | 2.4819 | — | Wet chlorine, mixed acids |
| Hastelloy C-22 | N06022 | — | 2.4602 | — | Oxidising + reducing media |
| Hastelloy B-2 | N10665 | — | 2.4617 | — | HCl and H₂SO₄ |
| Incoloy 800 / 800H | N08800 / N08810 | GH800 / GH800H | 1.4876 / 1.4959 | NCF800 / NCF800H | Reformer, cracking furnace |
| Incoloy 825 | N08825 | GH825 | 2.4858 | NCF825 | Sulphuric acid, seawater |
| Incoloy 925 | N09925 | — | — | — | Sour gas, age hardened |
| 0Cr25Al5 | — | 0Cr25Al5 (GB/T 1234) | — (Kanthal A-1 class) | FCH1 (approx.) | FeCrAl element wire, 1,300 °C |
| 0Cr27Al7Mo2 | — | 0Cr27Al7Mo2 (GB/T 1234) | — (no W.Nr.; FeCrAl, not MoSi₂) | FCH2 (approx.) | FeCrAl, 1,400 °C |
| Ni80Cr20 | N06003 | Cr20Ni80 (GB/T 1234) | NiCr 80/20 | NCH1 | Nichrome element wire |
| Ni60Cr15 | — | Cr15Ni60 | NiCr 60/15 | NCH2 | Nichrome, cost balanced |
| Constantan | — | 6J40 (CuNi40) / CuNi44 | 2.0842 | — | Precision resistance, T/C legs |
| Manganin | — | 6J13 | 2.0882 (CuMn12Ni) | — | Precision resistors |
| 4J29 | Kovar (ASTM F15) | 4J29 | 1.3981 | — | Glass-to-metal seal, Fe-29Ni-17Co |
| 4J36 | — | 4J36 | 1.3912 | — | Invar, Fe-36Ni, low expansion |
| ERNiCr-3 | N06082 | — | 2.4806 (NiCr20Mn3Nb) | — | Filler, Inconel 82 type |
| ERNiCrMo-3 | N06625 | — | 2.4831 (NiCr22Mo9Nb) | — | Filler, 625 type |
| ERNiCu-7 | N04019 | — | 2.4377 | — | Filler, Monel 60 type |
| ER308L / ER316L | S30883 / S31683 | H022Cr21Ni10 / H022Cr19Ni12Mo2 | 1.4316 / 1.4430 | YS308L / YS316L | Stainless filler |
| ER2209 | S39209 | — | 1.4462 | — | Duplex filler |
Equivalence is a starting point, not a guarantee. JIS designations follow JIS G 4901 / 4902 (NCF and NW series) and JIS C 2520 (NCH / FCH resistance wire); where JIS lists no grade we leave the cell blank rather than repeat the UNS number. FeCrAl has no EN Werkstoff number — Kanthal A-1 is a commercial grade of similar composition, not an equivalent, and Kanthal Super is a MoSi2 element, a different material family. Most nickel alloys map cleanly (Ni200 = N6 = 2.4060), but several Chinese grades have no exact Western counterpart: GH3030 and GH3128 are GB-specific superalloys, and 0Cr25Al5 is the GB designation for a Kanthal-type FeCrAl rather than a unified grade. Where the drawing calls for one system and the supplier stock uses another, ask for the heat chemistry and compare element by element — that comparison is exactly what we put on every quotation.
Can't find your grade? Send the chemical composition and service conditions instead of the name — we will match it to a stocked grade and put both analyses on the certificate.
Every cross-referenced grade has a TDS with chemistry, mechanicals and temperature data — request it from the download centre.