Elements rarely die of old age. They die at a specific spot, for a specific reason, and almost always for one of five reasons on this list. Every failure mode below is one our factory has replicated and diagnosed on real coils.

Surface load

The single biggest factor. Running a wire at 6 W/cm² instead of 4 W/cm² can halve life even though the alloy is comfortably within its temperature rating. If elements fail uniformly along their length, look here first.

Thermal cycling

Every heat-up grows the oxide scale; every cool-down cracks some of it off. Deep cycles (room temperature to full heat) are far more damaging than shallow ones. A slower start-up or a hold temperature overnight can double element life without any material change.

Atmosphere

FeCrAl depends on oxygen to maintain its alumina scale — in reducing atmospheres, vacuum or carbon-bearing environments, its surface degrades quickly and nichrome becomes the better choice. Sulphur and chlorine attack both families; halides attack nickel alloys specifically.

Support contact

The classic FeCrAl failure: sagging wire touches a ceramic or metal support, the contact point runs hot, and the wire thins there until it opens. Support spacing must follow the sag data of the specific grade at the actual service temperature — not a generic rule of thumb.

Contamination and mechanical damage

Drawing lubricant left on the wire, iron contamination from carbon-steel tools, or a kink from rough handling each create a local weak point. Contamination failures show up as isolated hot spots in the first hundred hours; they are almost always visible on the failed wire as a discoloured band.

Diagnosing from the failed wire

What you seeMost likely cause
Uniform thinning over the whole lengthSurface load too high
One thin spot at a supportSupport contact / spacing
Brittle fracture away from hot zonesGrain growth from over-temperature
Green or black deposit at failureAtmosphere contamination
Failure within hours of installationHandling damage or lubricant residue

Send us the failed wire with the operating history — temperature, atmosphere, cycle pattern and where it broke. In most cases we can name the cause from photographs and one measurement.

Key takeaways

  • Surface load is the first lever, not the last. Most premature failures are elements running hotter per unit area than the alloy can sustain in that atmosphere.
  • Thermal cycling consumes life in a way steady operation does not. Each cycle cracks and re-heals the oxide scale; short cycles are disproportionately damaging.
  • The support is part of the element. Contact points, ceramic quality and spacing determine whether the wire sags, shorts or locally overheats.
  • Read the failed wire before replacing it. Colour, sag pattern and break location each point to a different root cause — the replacement fails the same way if you skip this.

Frequently asked questions

What surface load should I design for?

It depends on alloy, atmosphere and whether the element is static or cyclic. As a rough guide, static FeCrAl elements in clean air can run higher than cyclic nichrome elements in the same chamber. Treat catalogue figures as ceilings, not targets, and derate for reducing atmospheres and frequent cycling.

Why did my element fail in three months when the last one lasted two years?

Check three things in order: whether the surface load changed (new element sized differently), whether the atmosphere changed (new process gas, sealing problem), and whether the support ceramics degraded. Grade substitution is a common fourth cause — a same-size replacement in a different alloy runs at a different wattage.

Do short heating cycles really shorten life?

Yes, disproportionately. Rapid cycling thermally shocks the oxide scale, causing spalling and re-growth that consumes aluminium or chromium from the alloy. Two thousand short cycles can do more damage than one long service period of the same total hours.

How do I tell overheating from contamination?

Overheating usually shows general sag, a dull or blistered surface and multiple breaks. Contamination tends to be local — a discoloured patch, a single break point, or attack where the element touches a support or refractory. Look at the break location first.

Is a thicker wire always longer-lived?

Only if the surface load stays the same or falls. A thicker wire at the same wattage and length runs cooler, which helps. But if the redesign raises the wattage, the surface load can go up and life goes down despite the extra metal.

D GO TOP Technical Team

Process Engineering · Wire Drawing & Heat Treatment

Our engineers support grade selection, element sizing and tolerance review for nickel, nickel-chromium, FeCrAl and superalloy wire. More about our technical team.

Next step

Send three numbers, get an answer

Diameter or cross-section, working temperature, and required power or resistance. We reply within 24 hours with the grade that fits, and with where the margin sits.

WhatsApp UsContact Us