A Turkish heat-treatment shop replaced nichrome elements that failed every 9 months with 0Cr25Al5 drawn to a matched resistance — and stopped planning shutdowns around element changes.
The customer ran two 1,150 °C annealing furnaces on Ni80Cr20 elements. Elements failed at the support points after roughly nine months: the wire sagged onto the supports, the local temperature rose, and the failure followed within weeks. Each change meant a full shift of downtime and an unplanned rush order for wire.
The failure was mechanical, not chemical. Sag data for Ni80Cr20 at 1,150 °C under that span length did not support the support spacing the furnace builder had used. The chemistry of the wire was fine — the design was asking the alloy to hold itself up longer than it could.
We quoted 0Cr25Al5 at the same resistance per metre, supplied with certified ±3% tolerance, together with a support-spacing recommendation from our sag trials. The element geometry was re-wound for the higher resistivity: shorter wire, slightly larger diameter, same wattage.
Application example, anonymised from our order book. Your numbers will differ with furnace design, atmosphere and cycle pattern — send them and we will size the element with you.
A cell assembler in Eastern Europe was seeing intermittent weld failures traced to strip thickness variation. …
ViewWeldingA fabricator building chemical piping in 2205 duplex needed filler wire with a ferrite balance that would surv…
ViewSend the application data — atmosphere, temperature, cycle and current specification. We will tell you what we would change and quote both options.